RefractiveIndex.INFO Refractive index database

Shelf

Book

Page

Optical constants of SCHOTT - LaSF (Lanthanum dense flint)
N-LASF43

Wavelength: µm
 (0.35 – 2.5)  
 

Other optical constants

n   k   logX   logY   eV

Dispersion formula [ i ]

$$n^2-1=\frac{1.93502827λ^2}{λ^2-0.0104001413}+\frac{0.23662935λ^2}{λ^2-0.0447505292}+\frac{1.26291344λ^2}{λ^2-87.437569}$$

Data

[Expressions for n]   [CSV - comma separated]   [TXT - tab separated]   [Full database record]

Additional information

n_is_absolute: false
λ_is_vacuum: false
temperature: 20.0 °C
coefficients_of_thermal_dispersion: 4.77e-06 1.14e-08 -2.68e-12 6.62e-07 8.84e-10 0.234
n_d: 1.8061
V_d: 40.61
glass_code: 806406.426
glass_status: standard
density: 4.26 g/cm3
coefficient_of_thermal_expansion_1: 5.49e-06 K-1
coefficient_of_thermal_expansion_2: 6.66e-06 K-1
ΔP_gF: -0.0052
climatic_resistance: 1.0
stain_resistance: 1.0
acid_resistance: 51.3
alkali_resistance: 1.0
phosphate_resistance: 2.0

References

1) SCHOTT optical glass data sheets 2015-07-22
2) SCHOTT Zemax catalog 2015-07-22

More info - wiki

SCHOTT AG is a German glass manufacturer. SCHOTT also publishes a glass catalog (SCHOTT Optical Glass Datasheets), which is a standard reference for the properties of many optical glasses.