RefractiveIndex.INFO Refractive index database

Shelf

Book

Page

Optical constants of SCHOTT - LaK (Lanthanum crown)
P-LAK35

Wavelength: µm
 (0.3 – 2.5)  
 

Other optical constants

n   k   logX   logY   eV

Dispersion formula [ i ]

$$n^2-1=\frac{1.3932426λ^2}{λ^2-0.00715959695}+\frac{0.418882766λ^2}{λ^2-0.0233637446}+\frac{1.043807λ^2}{λ^2-88.3284426}$$

Comments

suitable for precision molding

Data

[Expressions for n]   [CSV - comma separated]   [TXT - tab separated]   [Full database record]

Additional information

n_is_absolute: false
λ_is_vacuum: false
temperature: 20.0 °C
coefficients_of_thermal_dispersion: -1.9e-06 7.99e-09 7.76e-12 5.64e-07 6.57e-10 0.185
n_d: 1.6935
V_d: 53.2
glass_code: 693532.385
glass_status: standard
density: 3.848 g/cm3
coefficient_of_thermal_expansion_1: 8.13e-06 K-1
coefficient_of_thermal_expansion_2: 9.68e-06 K-1
ΔP_gF: -0.0061
climatic_resistance: 2.0
stain_resistance: 5.0
acid_resistance: 53.3
alkali_resistance: 1.3
phosphate_resistance: 4.3

References

1) SCHOTT optical glass data sheets 2015-07-22
2) SCHOTT Zemax catalog 2015-07-22

More info - wiki

SCHOTT AG is a German glass manufacturer. SCHOTT also publishes a glass catalog (SCHOTT Optical Glass Datasheets), which is a standard reference for the properties of many optical glasses.

External links