RefractiveIndex.INFO Refractive index database

Shelf

Book

Page

Optical constants of SCHOTT - LaK (Lanthanum crown)
N-LAK7

Wavelength: µm
 (0.29 – 2.5)  
 

Other optical constants

n   k   logX   logY   eV

Dispersion formula [ i ]

$$n^2-1=\frac{1.23679889λ^2}{λ^2-0.00610105538}+\frac{0.445051837λ^2}{λ^2-0.0201388334}+\frac{1.01745888λ^2}{λ^2-90.638038}$$

Data

[Expressions for n]   [CSV - comma separated]   [TXT - tab separated]   [Full database record]

Additional information

n_is_absolute: false
λ_is_vacuum: false
temperature: 20.0 °C
coefficients_of_thermal_dispersion: -3.4e-06 1.17e-08 2.38e-11 4.96e-07 4.44e-10 0.107
n_d: 1.6516
V_d: 58.52
glass_code: 652585.384
glass_status: standard
density: 3.84 g/cm3
coefficient_of_thermal_expansion_1: 7.1e-06 K-1
coefficient_of_thermal_expansion_2: 8.2e-06 K-1
ΔP_gF: -0.0021
climatic_resistance: 3.0
stain_resistance: 2.0
acid_resistance: 53.3
alkali_resistance: 3.3
phosphate_resistance: 4.3

References

1) SCHOTT optical glass data sheets 2015-07-22
2) SCHOTT Zemax catalog 2015-07-22

More info - wiki

SCHOTT AG is a German glass manufacturer. SCHOTT also publishes a glass catalog (SCHOTT Optical Glass Datasheets), which is a standard reference for the properties of many optical glasses.

External links