RefractiveIndex.INFO Refractive index database

Shelf

Book

Page

Optical constants of SCHOTT - LaK (Lanthanum crown)
N-LAK33A

Wavelength: µm
 (0.32 – 2.5)  
 

Other optical constants

n   k   logX   logY   eV

Dispersion formula [ i ]

$$n^2-1=\frac{1.44116999λ^2}{λ^2-0.00680933877}+\frac{0.571749501λ^2}{λ^2-0.0222291824}+\frac{1.16605226λ^2}{λ^2-80.9379555}$$

Comments

will become inquiry glass as of Jan 2015. not recommended for new design

Data

[Expressions for n]   [CSV - comma separated]   [TXT - tab separated]   [Full database record]

Additional information

n_is_absolute: false
λ_is_vacuum: false
temperature: 20.0 °C
coefficients_of_thermal_dispersion: 2.63e-06 1.11e-08 -3.92e-12 5.02e-07 5.08e-10 0.188
n_d: 1.75393
V_d: 52.27
glass_code: 754523.422
glass_status: standard
density: 4.216 g/cm3
coefficient_of_thermal_expansion_1: 5.8e-06 K-1
coefficient_of_thermal_expansion_2: 7.02e-06 K-1
ΔP_gF: -0.0086
climatic_resistance: 1.0
stain_resistance: 1.0
acid_resistance: 51.0
alkali_resistance: 1.0
phosphate_resistance: 2.0

References

1) SCHOTT optical glass data sheets 2015-07-22
2) SCHOTT Zemax catalog 2015-07-22

More info - wiki

SCHOTT AG is a German glass manufacturer. SCHOTT also publishes a glass catalog (SCHOTT Optical Glass Datasheets), which is a standard reference for the properties of many optical glasses.