RefractiveIndex.INFO Refractive index database

Shelf

Book

Page

Optical constants of SCHOTT - LaK (Lanthanum crown)
N-LAK12

Wavelength: µm
 (0.32 – 2.5)  
 

Other optical constants

n   k   logX   logY   eV

Dispersion formula [ i ]

$$n^2-1=\frac{1.17365704λ^2}{λ^2-0.00577031797}+\frac{0.588992398λ^2}{λ^2-0.0200401678}+\frac{0.978014394λ^2}{λ^2-95.4873482}$$

Data

[Expressions for n]   [CSV - comma separated]   [TXT - tab separated]   [Full database record]

Additional information

n_is_absolute: false
λ_is_vacuum: false
temperature: 20.0 °C
coefficients_of_thermal_dispersion: -5.67e-06 8.27e-09 1.27e-12 5.25e-07 6.3e-10 0.162
n_d: 1.6779
V_d: 55.2
glass_code: 678552.410
glass_status: standard
density: 4.1 g/cm3
coefficient_of_thermal_expansion_1: 7.6e-06 K-1
coefficient_of_thermal_expansion_2: 9.3e-06 K-1
ΔP_gF: -0.0024
climatic_resistance: 3.0
stain_resistance: 1.0
acid_resistance: 53.3
alkali_resistance: 3.3
phosphate_resistance: 4.3

References

1) SCHOTT optical glass data sheets 2015-07-22
2) SCHOTT Zemax catalog 2015-07-22

More info - wiki

SCHOTT AG is a German glass manufacturer. SCHOTT also publishes a glass catalog (SCHOTT Optical Glass Datasheets), which is a standard reference for the properties of many optical glasses.