RefractiveIndex.INFO Refractive index database

Shelf

Book

Page

Optical constants of SCHOTT - LLF (Very light flint)
LLF1HTi

Wavelength: µm
 (0.3 – 2.5)  
 

Other optical constants

n   k   logX   logY   eV

Dispersion formula [ i ]

$$n^2-1=\frac{1.22510445λ^2}{λ^2-0.00870432098}+\frac{0.125155671λ^2}{λ^2-0.0427325235}+\frac{0.892236751λ^2}{λ^2-108.049968}$$

Comments

i-line glass

Data

[Expressions for n]   [CSV - comma separated]   [TXT - tab separated]   [Full database record]

Additional information

n_is_absolute: false
λ_is_vacuum: false
temperature: 20.0 °C
coefficients_of_thermal_dispersion: 2.55e-07 1.41e-08 -3.32e-11 6.74e-07 6.27e-10 0.227
n_d: 1.54815
V_d: 45.9
glass_code: 548459.294
glass_status: standard
density: 2.94 g/cm3
coefficient_of_thermal_expansion_1: 8.1e-06 K-1
coefficient_of_thermal_expansion_2: 9.2e-06 K-1
ΔP_gF: -0.001
climatic_resistance: 1.0
stain_resistance: 0.0
acid_resistance: 1.0
alkali_resistance: 2.0
phosphate_resistance: 1.0

References

1) SCHOTT optical glass data sheets 2015-07-22
2) SCHOTT Zemax catalog 2015-07-22

More info - wiki

SCHOTT AG is a German glass manufacturer. SCHOTT also publishes a glass catalog (SCHOTT Optical Glass Datasheets), which is a standard reference for the properties of many optical glasses.