RefractiveIndex.INFO Refractive index database

Shelf

Book

Page

Optical constants of SCHOTT - KF (Crown/flint)
N-KF9

Wavelength: µm
 (0.35 – 2.5)  
 

Other optical constants

n   k   logX   logY   eV

Dispersion formula [ i ]

$$n^2-1=\frac{1.19286778λ^2}{λ^2-0.00839154696}+\frac{0.0893346571λ^2}{λ^2-0.0404010786}+\frac{0.920819805λ^2}{λ^2-112.572446}$$

Data

[Expressions for n]   [CSV - comma separated]   [TXT - tab separated]   [Full database record]

Additional information

n_is_absolute: false
λ_is_vacuum: false
temperature: 20.0 °C
coefficients_of_thermal_dispersion: -1.66e-06 8.44e-09 -1.01e-11 6.1e-07 6.96e-10 0.217
n_d: 1.52346
V_d: 51.54
glass_code: 523515.250
glass_status: standard
density: 2.499 g/cm3
coefficient_of_thermal_expansion_1: 9.61e-06 K-1
coefficient_of_thermal_expansion_2: 1.095e-05 K-1
ΔP_gF: -0.0014
climatic_resistance: 1.0
stain_resistance: 0.0
acid_resistance: 1.0
alkali_resistance: 1.0
phosphate_resistance: 1.0

References

1) SCHOTT optical glass data sheets 2015-07-22
2) SCHOTT Zemax catalog 2015-07-22

More info - wiki

SCHOTT AG is a German glass manufacturer. SCHOTT also publishes a glass catalog (SCHOTT Optical Glass Datasheets), which is a standard reference for the properties of many optical glasses.