RefractiveIndex.INFO Refractive index database

Shelf

Book

Page

Optical constants of SCHOTT - FK (Fluorite crown)
N-FK5

Wavelength: µm
 (0.26 – 2.5)  
 

Other optical constants

n   k   logX   logY   eV

Dispersion formula [ i ]

$$n^2-1=\frac{0.844309338λ^2}{λ^2-0.00475111955}+\frac{0.344147824λ^2}{λ^2-0.0149814849}+\frac{0.910790213λ^2}{λ^2-97.8600293}$$

Comments

suitable for precision molding. step 0.5 available

Data

[Expressions for n]   [CSV - comma separated]   [TXT - tab separated]   [Full database record]

Additional information

n_is_absolute: false
λ_is_vacuum: false
temperature: 20.0 °C
coefficients_of_thermal_dispersion: -7.24e-06 1.58e-08 -9.51e-12 3.51e-07 4.61e-10 0.156
n_d: 1.48749
V_d: 70.41
glass_code: 487704.245
glass_status: standard
density: 2.45 g/cm3
coefficient_of_thermal_expansion_1: 9.2e-06 K-1
coefficient_of_thermal_expansion_2: 1e-05 K-1
ΔP_gF: 0.0036
climatic_resistance: 2.0
stain_resistance: 1.0
acid_resistance: 4.0
alkali_resistance: 2.0
phosphate_resistance: 2.3

References

1) SCHOTT optical glass data sheets 2015-07-22
2) SCHOTT Zemax catalog 2015-07-22

More info - wiki

SCHOTT AG is a German glass manufacturer. SCHOTT also publishes a glass catalog (SCHOTT Optical Glass Datasheets), which is a standard reference for the properties of many optical glasses.