RefractiveIndex.INFO Refractive index database

Shelf

Book

Page

Optical constants of SCHOTT - FK (Fluorite crown)
FK5HTi

Wavelength: µm
 (0.25 – 2.5)  
 

Other optical constants

n   k   logX   logY   eV

Dispersion formula [ i ]

$$n^2-1=\frac{0.90936218λ^2}{λ^2-0.0052014247}+\frac{0.279077054λ^2}{λ^2-0.0158938446}+\frac{0.891813298λ^2}{λ^2-95.9109448}$$

Comments

i-line glass

Data

[Expressions for n]   [CSV - comma separated]   [TXT - tab separated]   [Full database record]

Additional information

n_is_absolute: false
λ_is_vacuum: false
temperature: 20.0 °C
coefficients_of_thermal_dispersion: -7.47e-06 1.58e-08 -1.23e-11 3.58e-07 4.03e-10 0.164
n_d: 1.48748
V_d: 70.47
glass_code: 487705.245
glass_status: standard
density: 2.45 g/cm3
coefficient_of_thermal_expansion_1: 9.2e-06 K-1
coefficient_of_thermal_expansion_2: 1e-05 K-1
ΔP_gF: 0.0036
climatic_resistance: 2.0
stain_resistance: 1.0
acid_resistance: 4.0
alkali_resistance: 2.0
phosphate_resistance: 2.3

References

1) SCHOTT optical glass data sheets 2015-07-22
2) SCHOTT Zemax catalog 2015-07-22

More info - wiki

SCHOTT AG is a German glass manufacturer. SCHOTT also publishes a glass catalog (SCHOTT Optical Glass Datasheets), which is a standard reference for the properties of many optical glasses.