RefractiveIndex.INFO Refractive index database

Shelf

Book

Page

Optical constants of SCHOTT - BaK (Barium crown)
N-BAK2

Wavelength: µm
 (0.3 – 2.5)  
 

Other optical constants

n   k   logX   logY   eV

Dispersion formula [ i ]

$$n^2-1=\frac{1.01662154λ^2}{λ^2-0.00592383763}+\frac{0.319903051λ^2}{λ^2-0.0203828415}+\frac{0.937232995λ^2}{λ^2-113.118417}$$

Data

[Expressions for n]   [CSV - comma separated]   [TXT - tab separated]   [Full database record]

Additional information

n_is_absolute: false
λ_is_vacuum: false
temperature: 20.0 °C
coefficients_of_thermal_dispersion: -1.45e-06 1.1e-08 4.89e-12 5.16e-07 3.05e-10 0.164
n_d: 1.53996
V_d: 59.71
glass_code: 540597.286
glass_status: standard
density: 2.86 g/cm3
coefficient_of_thermal_expansion_1: 8e-06 K-1
coefficient_of_thermal_expansion_2: 9e-06 K-1
ΔP_gF: 0.0004
climatic_resistance: 2.0
stain_resistance: 0.0
acid_resistance: 1.0
alkali_resistance: 1.0
phosphate_resistance: 2.3

References

1) SCHOTT optical glass data sheets 2015-07-22
2) SCHOTT Zemax catalog 2015-07-22

More info - wiki

SCHOTT AG is a German glass manufacturer. SCHOTT also publishes a glass catalog (SCHOTT Optical Glass Datasheets), which is a standard reference for the properties of many optical glasses.

External links