Optical constants of OHARA - FPL (Fluorophosphate, low-index)
S-FPL53

Wavelength: µm
 (0.28 – 2.4)  
 

Other optical constants

n   k   logX   logY   eV

Dispersion formula [ i ]

$$n^2-1=\frac{0.983532327λ^2}{λ^2-0.00492234955}+\frac{0.069568814λ^2}{λ^2-0.0193581091}+\frac{1.11409238λ^2}{λ^2-264.275294}$$

Comments

Recommended -The unique relative partial dispersion.

Data

[Expressions for n]   [CSV - comma separated]   [TXT - tab separated]   [Full database record]

Additional information

n_is_absolute: false
λ_is_vacuum: false
temperature: 25.0 °C
coefficients_of_thermal_dispersion: -2.22e-05 -1.06e-08 -4.91e-11 2.77e-07 3.92e-10 0.206
n_d: 1.438750
V_d: 94.946025
glass_code: 439950
glass_status: standard
density: 3.62 g/cm3
coefficient_of_thermal_expansion_1: 1.45e-05 K-1
coefficient_of_thermal_expansion_2: 1.69e-05 K-1
ΔP_gF: 0.0461
climatic_resistance: 3.0
acid_resistance: 52.3
phosphate_resistance: 4.3

References

1) OHARA optical glass datasheets 2015-12-01
2) OHARA Zemax catalog 2015-12-01

More info - wiki

Ohara Group is an international group of companies with headquarters in Japan and subsidiaries in Japan (Ohara, Inc.), United States (Ohara Corporation), and Germany (Ohara, GmbH). Ohara manufactures optical and electronic products and also offers measurement services, in particular measurement of refractive indices of solids and liquids.